牌號
|
X4CrNiMo16-5-1壓力容器用不銹鋼扁平
|
|
|
|
|
|
|
|
|
|
1.4418
|
|
|
|
|
|
|
|
|
對應標準
|
NF EN 10028-7-2008
|
|
|
|
|
|
|
|
|
壓力容器用不銹鋼扁平產品
|
|
|
|
|
|
|
|
|
Flat products made of steels for pressure purposes - Part 7 : stainless steels
|
|
|
|
|
|
|
|
|
歸類
|
馬氏體不銹鋼
|
|
|
|
|
|
|
|
|
X4CrNiMo16-5-1 化學元素成分含量(%)
|
|
|
|
|
|
|
|
|
|
成分
|
C
|
Si
|
Mn
|
P
|
S
|
Cr
|
Ni
|
Mo
|
N
|
最小值
|
-
|
-
|
-
|
-
|
-
|
15
|
4
|
0.8
|
0.02
|
最DA值
|
0.06
|
0.7
|
1.5
|
0.04
|
0.015
|
17
|
6
|
1.5
|
-
|
◎ 未經買方同意,不得隨意向鋼中添加表中未列的元素,冶煉精加工除外。采取一切必要措施以防在廢鋼和生產原料中帶入這些元素,因為其會削弱鋼的機械性能,降低鋼的適用性。
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
X4CrNiMo16-5-1 機械性能
|
|
|
|
|
|
|
|
|
|
條件
|
熱處理或狀態
|
抗拉強度
|
屈服點
|
斷后伸長率或延伸率
|
沖擊吸收能量
|
|
|
|
|
σb
|
σs
|
δ
|
KV2
|
|
|
|
|
Mpa
|
Mpa
|
%
|
J
|
|
|
|
|
P:T ≤ 75
|
+QT
|
840~980
|
≥680
|
14 ①
|
20℃: ≥ 55
|
|
|
|
|
-20℃: ≥ 40
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
◎C- 冷軋帶鋼; H- 熱軋帶鋼; P- 熱軋中厚板;T- 厚度;t- 橫向;l-縱向。
|
|
|
|
|
|
|
|
|
|
◎+A=軟化退火;+AT=固溶退火;+QT=淬火及回火;+RA=再結晶退火。
|
|
|
|
|
|
|
|
|
|
① T ≥3mm:該值適用于標距為5.65√S的試件。
|
|
|
|
|
|
|
|
|
|