牌號
|
1.4550壓力容器用不銹鋼扁平
|
|
|
|
|
|
|
|
|
X6CrNiNb 18-10
|
|
|
|
|
|
|
|
對應標準
|
NF EN 10028-7-2008
|
|
|
|
|
|
|
|
壓力容器用不銹鋼扁平產品
|
|
|
|
|
|
|
|
Flat products made of steels for pressure purposes - Part 7 : stainless steels
|
|
|
|
|
|
|
|
歸類
|
奧氏體不銹鋼
|
|
|
|
|
|
|
|
標簽
|
耐腐蝕等級
|
|
|
|
|
|
|
|
X6CrNiNb18-10 化學元素成分含量(%)
|
|
|
|
|
|
|
|
|
成分
|
C
|
Si
|
Mn
|
P
|
S
|
Cr
|
Ni
|
更多
|
最小值
|
-
|
-
|
-
|
-
|
-
|
17
|
9
|
Nb:10×C~1
|
最DA值
|
0.08
|
1
|
2
|
0.045
|
0.015
|
19
|
12
|
◎ 未經買方同意,不得隨意向鋼中添加表中未列的元素,冶煉精加工除外。采取一切必要措施以防在廢鋼和生產原料中帶入這些元素,因為其會削弱鋼的機械性能,降低鋼的適用性。
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
X6CrNiNb18-10 機械性能
|
|
|
|
|
|
|
|
|
條件
|
熱處理或狀態
|
抗拉強度
|
屈服點
|
斷后伸長率或延伸率
|
沖擊吸收能量
|
|
|
|
σb
|
σs
|
δ
|
KV2
|
|
|
|
Mpa
|
Mpa
|
%
|
J
|
|
|
|
H:T ≤ 13.5
|
+AT
|
520~720
|
Rp0.2:≥200
|
T < 3mm: ≥40
|
20℃:
|
|
|
|
Rp1.0:≥240
|
T ≥ 3mm: ≥ 40
|
(l: ≥100;t: ≥60)
|
|
|
|
①②
|
②③
|
-196℃:
|
|
|
|
|
|
(t: ≥40)
|
|
|
|
P:T ≤ 75
|
+AT
|
500~700
|
Rp0.2:≥200
|
T < 3mm: ≥40
|
20℃:
|
|
|
|
Rp1.0:≥240
|
T ≥ 3mm: ≥ 40
|
(l: ≥100;t: ≥60)
|
|
|
|
①②
|
②③
|
-196℃:
|
|
|
|
|
|
(t: ≥40)
|
|
|
|
◎C- 冷軋帶鋼; H- 熱軋帶鋼; P- 熱軋中厚板;T- 厚度;t- 橫向;l-縱向。
|
|
|
|
|
|
|
|
|
◎+A=軟化退火;+AT=固溶退火;+QT=淬火及回火;+RA=再結晶退火。
|
|
|
|
|
|
|
|
|
◎ 奧氏體鋼有足夠的韌性,不需要進行沖擊試驗。相比之下,奧氏體-鐵素體鋼必須按要求做沖擊試驗,以確保足夠的韌性。
|
|
|
|
|
|
|
|
|
*抗晶間腐蝕根據EN ISO 3651-2進行測試。在交貨條件下:有;在致敏狀態下:有。
|
|
|
|
|
|
|
|
|
① 對于連續熱軋產品,可在詢價和訂購時商定Rp0.2(即表中σs)的最小值提高20MPa,Rp1.0的最小值提高10MPa。
|
|
|
|
|
|
|
|
|
② 如果在軋制寬度<300mm的帶材情況下,采用縱向試驗件,最小值減小如下:抗拉強度-15MPa,恒定標距的延伸率-5%,比例標距延伸率-2%。
|
|
|
|
|
|
|
|
|
③ T<3mm:該值適用于標距為80mm、寬度為20mm的試件,也可以使用標距為50mm、寬度為12.5mm的試件。T ≥3mm:該值適用于標距為5.65√S的試件。
|
|
|
|
|
|
|
|
|