磷銅釬料主要技術參數 Technical Characteristics of copper-phosphorus alloys: | |||||||
釬料牌號 Brazing Alloys |
主要化學成份 (%) Chemical Composition |
熔化溫度℃ Melting range ℃ |
焊接溫度℃ Working temperture℃ |
強度(N/mm) Trensile |
相當于其它 標準牌號 Ref. code in other standards |
公司代號 Huazhong code | |
Б | t | ||||||
BCu95P | Cu:95;P:5 | 778~924℃ | 788~927℃ | AWS BCuP-1 |
95P | ||
BCu94P | Cu:94;P:6 | 750~880℃ | 743~840℃ | 94P | |||
BCu93P | Cu:93;P:7 | 710~800℃ | 743~840℃ | 150 160 |
160 200 |
AWS BCuP-2 China HL202 |
93P |
BCu92P | Cu:92;P:8 | 710~780℃ | 730~830℃ | 141 156 |
151 200 |
China HL201 | 92P |
BCu86PSn | Cu:86;P:7;Sn:7 | 640~680℃ | 700~750℃ | / | / | China HL208 | 86PS |
BCu90PSn | Cu:90;P:6.5; Sn:4.5 |
650~700℃ | 710~760℃ | / | / | 90PS | |
BCu75PSnNi | Cu:75;Sn15 P、Ni等; |
590~600℃ | 600~650℃ | / | / | 75PS | |
BCu91PSb | Cu:90;P:7;Sb:2 | 650~700℃ | 710~760℃ | 150 176 |
167 224 |
China HL203 | |
BCu92PAg | Cu:92;P:7;Ag:1 | 645~780℃ | 740~810℃ | / | / | 1B | |
BCu91PAg | Cu:91;P:7;Ag:2 | 643~778℃ | 730~810℃ | 190 200 |
170 180 |
Japan BCuP-6 China HL209 |
2B |
BCu90PAg | Cu:90;P:7;Ag:3 | 643~843℃ | 710~850℃ | / | / | 3B | |
![]() | |||||||
BCu88PAg | Cu:88;P:6.5;Ag:5 | 643~843℃ | 705~850℃ | 180 200 |
169 320 |
AWS BCuP-7 | 5B |
BCu89PAg | Cu:89;P:6;Ag:5 | 643~843℃ | 705~850℃ | 180 200 |
169 320 |
AWS BCuP-3 China HL205 |
5B-1 |
BCu87PAg | Cu:87;P:7;Ag:6 | 645~725℃ | 705~780℃ | / | / | AWS BCuP-4 | 6B |
BCu80PAg | Cu:80;P:5;Ag:15 | 643~802℃ | 704~810℃ | 188 228 |
163 340 |
AWS BCuP-5 | 15B |
BCu75PAg | Cu:75;P:7;Ag:18 | 640~670℃ | 704~810℃ | 188 228 |
163 340 |
18B | |
應用說明 Applications |
· BCuP類釬料主要用于釬接銅和銅合金,用于銀、鎢和鉬則受到一些限制。 · 這類釬料不得用于鐵基或鎳基合金和含鎳量超過10%的銅-鎳合金。 · BCuP類釬料適用于所有的釬焊方法,接頭形式推薦采用搭接接頭。 · 釬焊純銅(紫銅)時,BCuP類釬料可以不用釬劑;但是釬焊其他所有金屬時(包括銅合金), 則建議與釬劑配合使用。 · 釬焊前必須嚴格清除釬焊表面的油脂、氧化物等污物,釬焊接頭最好間隙為0.03~0.075mm。 · 釬焊后接頭顏色呈淺灰色,浸入10%的硫酸溶液中可恢復銅的顏色。 |